What are the characteristics, main alloying elements and functions of 2xxx series aluminum alloys?
(1) Characteristics of 2xxx series aluminum alloys
2xxX series aluminum alloys are aluminum alloys with copper as the main alloying element. They include Al-Cu-Mg alloys, Al-Cu-Mg-Fe-Ni alloys and Al-Cu-Mn alloys. These alloys are heat-treated aluminum alloys.
2xXX series aluminum alloys are characterized by high strength and are usually called hard aluminum alloys. They have good heat resistance and processing properties, but their corrosion resistance is not as good as most other aluminum alloys. Under certain conditions, intergranular corrosion will occur. Therefore, the plate often needs to be coated with a layer of pure aluminum or a layer of 6xXx series aluminum alloy that has electrochemical protection for the core plate to greatly improve its corrosion resistance. Among them, Al-Cu-Mg-Fe-Ni alloy has extremely complex chemical composition and phase composition. It has high strength at high temperature and good process performance. It is mainly used for heat-resistant parts working below 150~250℃; although the room temperature strength of AI-Cu-Mn alloy is lower than that of Al-Cu-Mg alloy 2A12 and 2A14, its strength is higher than both at 225~250℃ or higher. In addition, the alloy has good process performance and is easy to weld. It is mainly used in heat-resistant weldable structural parts and forgings. This series of alloys are widely used in aviation and aerospace fields.

(2) Main alloying elements and their roles
①The main alloy grades of AI-Cu-Mg alloys are 2A01, 2A02, 2A06, 2A10, 2A11, 2A12, etc. The main added elements are Cu, Mg and Mn.
Their effects on the alloys are as follows.
a. Effect of Cu and Mg content on the mechanical properties of the alloys. When the Mg content is 1%~2%, when the Cu content increases from 1.0% to 4%, the tensile strength of the alloy in the quenched state increases from 200MPa to 380MPa; the tensile strength of the alloy in the quenched natural aging state increases from 300MPa to 480MPa. When the Cu content is in the range of 1%~4%, when the Mg content increases from 0.5% to 2.0%, the tensile strength of the alloy increases; when the Mg content continues to increase, the strength of the alloy decreases.
The tensile strength of the alloy containing 4.0% Cu and 2.0% Mg is the highest; the alloy containing 3%~4% Cu and 0.5%~1.3% Mg has the greatest quenching and natural aging effect. The test shows that the tensile strength of the AI-Cu-Mg ternary alloy containing 4%~6% Cu and 1%~2% Mg can reach 490~510MPa in the quenching and natural aging state.
b. The influence of Cu and Mg content on the heat resistance of the alloy. From the endurance strength test values of AI-Cu-Mg alloy containing 0.6%Mn at 200℃ and 160MPa stress, it can be seen that the alloy containing Cu 3.5%~6% and Mg1.2%~2.0% has the highest endurance strength. At this time, the alloy is located on or near the AI-S (AlCuMg) pseudo-binary section. The alloy away from the pseudo-binary section, that is, when the Mg content is less than 1.2% and the maximum strength is greater than 2.0%, its endurance strength decreases. If the Mg content is increased to 3.0% or more, the alloy endurance strength will decrease rapidly.
Similar rules were obtained in the test at 250℃ and 100MPa stress. The literature points out that the alloy with the highest endurance strength at 300℃ is located in the α+S phase region to the right of the AI-S binary section with a higher Mg content.
c. Effect of Cu and Mg content on corrosion resistance of alloys. Al-Cu binary alloys with Cu content of 3%~5% have very low corrosion resistance in the state of quenching and natural aging. Adding 0.5%Mg can reduce the potential of a solid solution and partially improve the corrosion resistance of the alloy. When the Mg content is greater than 1.0%, the local corrosion of the alloy increases, and the elongation after corrosion decreases sharply. For alloys with Cu content greater than 4.0% and Mg content greater than 1.0%, Mg reduces the solubility of Cu in Al. In the quenched state, the alloy has insoluble CuAl₂ and S phases, and the presence of these phases accelerates corrosion. Alloys with Cu content of 3%~5% and Mg content of 1%~4% are located in the same phase region, and their corrosion resistance is similar in the state of quenching and natural aging. The alloys in the a-S phase region have poorer corrosion resistance than those in the a-CuAl₂-S region. Intergranular corrosion is the main corrosion tendency of Al-Cu-Mg alloys.
Mn: Mn is added to Al-Cu-Mg alloy mainly to eliminate the harmful effects of Fe and improve corrosion resistance. Mn can slightly increase the room temperature strength of the alloy, but reduce the plasticity. Mn can also delay and weaken the artificial aging process of Al-Cu Mg alloy and improve the heat resistance of the alloy. Mn is also one of the main factors that make Al-Cu-Mg alloy have extrusion effect. The addition of Mn is generally less than 1.0%. If the content is too high, coarse (FeMn)Al6 brittle compounds can be formed, reducing the plasticity of the alloy.
d. The small amount of trace elements added to Al-Cu-Mg alloys include Ti and Zr, and the impurities are mainly Fe, Si and Zn, etc., and their effects are as follows.
Ti: Adding Ti to the alloy can refine the cast grains and reduce the tendency to form cracks during casting.
Zr: A small amount of Zr has a similar effect to Ti, refining the cast grains, reducing the tendency to crack in casting and welding, and improving the plasticity of ingots and welded joints. Adding Zr does not affect the strength of cold-deformed products containing Mn alloys
It slightly improves the strength of Mn-free alloys. Si: For Al-Cu-Mg alloys with Mg content less than 1.0%, Si content exceeding 0.5% can improve the speed and strength of artificial aging without affecting the natural aging ability. Because Si and Mg form Mg2Si phase, it is beneficial to the artificial aging effect. However, when the Mg content is increased to 1.5%, after quenching natural aging or artificial aging treatment, the strength and heat resistance of the alloy decrease with the increase of Si content. Therefore, the Si content should be reduced as much as possible. In addition, the increase in Si content will increase the tendency of alloys such as 2A12 and 2A06 to form cracks during casting, and reduce plasticity during riveting. Therefore, the Si content in the alloy is generally limited to less than 0.5%. For alloys requiring high plasticity, the Si content should be lower.
Fe: Fe and Al form FeAl3 compounds and dissolve in compounds formed by elements such as Cu, Mn, and Si. These coarse compounds that do not dissolve in the solid solution reduce the plasticity of the alloy, and the alloy is prone to cracking during deformation. And the strengthening effect is significantly reduced. A small amount of Fe (less than 0.25%) has little effect on the mechanical properties of the alloy, improves the tendency of crack formation during casting and welding, but reduces the natural aging rate. In order to obtain highly plastic materials, the Fe and Si contents in the alloy should be as low as possible.
Zn: A small amount of Zn (0.1%~0.5%) has little effect on the room temperature mechanical properties of Al-Cu-Mg alloys, but reduces the heat resistance of the alloy. The Zn content in the alloy should be limited to less than 0.3%.
② Al-Cu-Mg-Fe-Ni alloy The main alloy grades of this series of alloys are 2A70, 2A80, 2A90, etc. The role of each alloy element is as follows.
Cu and Mg: The influence of Cu and Mg content on the room temperature strength and heat resistance of the above alloys is similar to that of AI-Cu-Mg alloy. Since the Cu and Mg content in this series of alloys is lower than that of AI-Cu-Mg alloy, the alloy is located in the a+ S (AlCuMg) two-phase region, so the alloy has higher room temperature strength and good heat resistance; in addition, when the Cu content is low, the low-concentration solid solution has a small tendency to decompose, which is beneficial to the heat resistance of the alloy.
Ni: Ni and Cu in the alloy can form an insoluble ternary compound. When the Ni content is low, (AICuNi) is formed, and when the Ni content is high, Al3(CuNi)2 is formed. Therefore, the presence of Ni can reduce the concentration of Cu in the solid solution. The measurement results of the lattice constant in the quenched state also prove the depletion of Cu solute atoms in the alloy solid solution. When the Fe content is very low, the increase in Ni content can reduce the hardness of the alloy and reduce the strengthening effect of the alloy.
Fe: Like Ni, Fe can also reduce the concentration of Cu in the solid solution. When the nickel content is very low, the hardness of the alloy decreases significantly at the beginning with the increase of Fe content, but when the Fe content reaches a certain value, it begins to increase again.
Ni and Fe: When Fe and Ni are added to the AICu2.2Mg1.65 alloy at the same time, the hardness change characteristics under quenching natural aging, quenching artificial aging, quenching and annealing are similar, and a maximum value appears at the position where the Ni and Fe contents are similar, and the lattice constant in the quenching state appears a minimum value at this point.
When the Fe content in the alloy is greater than the Ni content, Al7Cu2Fe phase will appear. On the contrary, when the Ni content in the alloy is greater than the Fe content, AlCuNi phase will appear. The appearance of the above Cu-containing ternary phase reduces the Cu content in the solid solution. Only when the Fe and Ni contents are equal, all AlgFeNi phases are generated. In this case, since there is no excess Fe or Ni to form an insoluble Cu-containing phase, the Cu in the alloy not only forms the S (Al2CuMg) phase, but also increases the concentration of Cu in the solid solution, which is beneficial to improving the strength of the alloy and its heat resistance.
Fe and Ni content can affect the heat resistance of the alloy. The AlgFeNi phase is a hard and brittle compound with very little solubility in Al. After forging and heat treatment, when they are dispersed and distributed in the structure, they can significantly improve the heat resistance of the alloy. For example, the AICu2.2Mg1.65 alloy contains 1.0% Ni and the alloy with 0.7%~0.9% Fe has the highest enduring strength value.
Si: Adding 0.5% to 1.2% Si to 2A80 alloy improves the room temperature strength of the alloy, but reduces the heat resistance of the alloy.
Adding 0.02%~0.1% Ti to Ti:2A70 alloy refines the as-cast grains and improves forging process performance, which is beneficial to heat resistance, but has little effect on room temperature performance.
③ Al-Cu-Mn alloy. The main alloy grades of this series of alloys are 2A16, 2A17, etc.
The functions of the main alloying elements are as follows.
Cu: At room temperature and high temperature, as the Cu content increases, the alloy strength increases. When the Cu content reaches 5.0%, the alloy strength is close to the maximum value. In addition, Cu can improve the welding performance of the alloy.
Mn: Mn is the main element to improve the heat-resistant alloy. It increases the activation energy of atoms in the solid solution, reduces the diffusion coefficient of solute atoms and the decomposition rate of the solid solution. When the solid solution decomposes, the formation and growth process of the precipitated phase T (Al2oCu2Mn3) phase is also very slow, so the alloy is also very stable when heated for a long time at a certain high temperature. Adding appropriate Mn (0.6%~0.8%) can improve the room temperature strength and endurance strength of the alloy in the quenching and natural aging state. However, if the Mn content is too high, the T phase increases, the interface increases, the diffusion effect is accelerated, and the heat resistance of the alloy is reduced. In addition, Mn can also reduce the crack tendency during alloy welding.
The trace elements added to Al-Cu-Mn alloy are Mg, Ti and Zr, while the main impurity elements are Fe, Si, Zn, etc., and their effects are as follows.
Mg: When the content of Cu and Mn in 2A16 alloy remains unchanged, 0.25%~0.45% Mg is added to form 2A17 alloy. Mg can improve the room temperature strength of the alloy and improve the heat resistance below 150~225℃. However, when the temperature rises further, the strength of the alloy decreases significantly. However, the addition of Mg can deteriorate the welding performance of the alloy, so in the 2A16 alloy used for heat-resistant weldability, the content of impurity Mg should not exceed 0.05%. Ti: Ti can refine the cast grains, increase the recrystallization temperature of the alloy, reduce the decomposition tendency of the supersaturated solid solution, and stabilize the structure of the alloy at high temperature. However, when the Ti content is greater than 0.3%, coarse needle-shaped TiAls compounds are generated, which reduces the heat resistance of the alloy. The Ti content of the alloy is specified to be 0.1%~0.2%. Zr: When 0.1%~0.25% Zr is added to 2219 alloy, the grains can be refined, and the recrystallization temperature and solid solution stability of the alloy can be increased, thereby improving the heat resistance of the alloy, and improving the weldability of the alloy and the plasticity of the weld. However, when the Zr content is high, more brittle compounds ZrAl3 can be generated.
Fe: When the Fe content in the alloy exceeds 0.45%, an insoluble phase AlCu2Fe is formed, which can reduce the mechanical properties of the alloy in the quenching and aging state and the endurance strength at 300°C. Therefore, the Fe content should be limited to less than 0.3%.
Si: A small amount of Si (0.4%) has no obvious effect on the room temperature mechanical properties, but reduces the endurance strength at 300°C. When the Si content exceeds 0.4%, the room temperature mechanical properties of the alloy will be reduced. Therefore, the Si content is limited to less than 0.3%.
Zn: A small amount of Zn (0.3%) has no effect on the room temperature properties of the alloy, but it can accelerate the diffusion rate of Cu in Al and reduce the endurance strength of the alloy at 300°C, so it is limited to less than 0.1%.

What are the types and uses of 2xxx series aluminum alloys?
Alloy 2011
Types: wire drawing tubes, cold-worked bars, cold-worked wires
Applications: screws and machined products requiring good cutting performance
Alloy 2014
Types: plates, thick plates, drawn tubes, extruded tubes, bars, profiles, wires, cold-worked bars, cold-worked wires, forgings
Applications: used in applications requiring high strength and hardness (including high temperatures). Heavy forgings, thick plates and extruded materials are used for aircraft structural parts, multi-stage rocket first-stage fuel tanks and spacecraft parts, wheels, truck frames and suspension system parts
Alloy 2017
Types: plates, extruded profiles, cold-worked bars, cold-worked wires, rivet wires, forgings
Applications: It is the first 2XXX series alloy to be industrially applied. Its current application range is relatively narrow, mainly rivets, general machinery parts, aircraft, ships, transportation, building structural parts, transportation vehicle structural parts, propellers and accessories
Alloy 2024
Varieties: Plates, thick plates, drawn tubes, extruded tubes, profiles, bars, wires, cold-worked bars, cold-worked wires, rivet wires
Applications: Aircraft structures (skins, frames, ribs, bulkheads, etc.), rivets, missile components, truck wheels, propeller components and other various structural parts
Alloy 2036
Varieties: Automotive body sheets
Applications: Automotive body sheet metal parts
Alloy 2048
Varieties: Plates
Applications: Aerospace structural parts and weapon structural parts
Alloy 2117
Varieties: Cold-worked bars and wires, rivet wires
Applications: Used as rivets for structural parts with working temperatures not exceeding 100°C
Alloy 2124
Varieties: Thick plates
Applications: Aerospace structural parts
Alloy 2218
Varieties: Forgings, foils
Applications: Aircraft engine and diesel engine pistons, aircraft engine cylinder heads, jet engine impellers and compressor rings
Alloy 2219
Varieties: Plates, thick plates, foils, extruded tubes, profiles, bars, wires, cold-worked bars, forgings
Applications: Space rocket welding oxidizer tanks and fuel tanks, supersonic aircraft skins and structural parts, operating temperature -270~300℃. Good weldability, high fracture toughness, high resistance to stress corrosion cracking in T8 state

Alloy 2319
Variety: Wire
Application: Welding rods and filler solder for welding 2219 alloy
Alloy 2618
Variety: Thick plates, extruded bars, forgings and forgings
Application: Engine cylinders and other parts, as well as heat-resistant parts that require working at 150~250℃. Thick plates are used as aircraft skins, bars, die forgings and free forgings are used to make pistons, aviation
Alloy 2A01
Variety: Cold-worked bars and wires, rivet wires
Application: Used as rivets for structural parts with working temperatures not exceeding 100℃
Alloy 2A02
Variety: Bars, forgings
Application: Axial compressor blades, impellers and disks of turbojet engines with working temperatures of 200~300℃
Alloy 2A04
Variety: Rivet wires
Application: Used to make rivets for structural parts with working temperature of 120~250℃
Alloy 2A06
Variety: Plate, extruded profile, rivet wire
Application: Aircraft structural parts with working temperature of 150~250℃ and aircraft structural rivets with working temperature of 125~250℃
Alloy 2A10
Variety: Rivet wire
Application: Higher strength than 2A01 alloy, used to manufacture aircraft structural rivets with working temperature ≤100℃
Alloy 2A50
Variety: Forgings, bars, plates
Application: Medium-strength parts with complex shapes
Alloy 2B50
Variety: Forgings
Application: Aircraft engine compressor wheel, guide wheel, fan, impeller, etc.
Alloy 2A90
Variety: Extruded bars, forgings and forgings
Application: Aircraft engine parts and other parts with high working temperature, alloy forgings are gradually replaced by 2A70