The raw materials used for coated aluminum coils are industrial high-purity aluminum coils, and the purity is required to be above 99.93% (mass fraction). Among them, the mass fraction of Al in the coated aluminum coils is required to be above 99.99%. The impurity elements in industrial high-purity aluminum include Fe, Si, Cu, Mg, Zn, Mn, Ni, Ti, etc., among which Fe, Si, and Cu are the main ones. The purity of high-purity aluminum can affect its recovery temperature. During the annealing process, the solid solution atoms of its impurity elements are distributed at sub-grain boundaries, which can hinder grain boundary migration, thereby affecting the growth of cubic-oriented grains, thereby affecting the performance of electrolytic capacitors. The current international trend is to require lower contents of Fe, Si, and Cu in aluminum coils for electrolytic capacitors, while strictly controlling the contents of other impurity elements.

 

aluminum-coating-coil

 

(1) The influence of Fe.

Fe is the most harmful impurity element in high-purity aluminum. Its content and distribution shape can affect the performance of coated aluminum coils. Fe generally exists in solid solution form in high-purity aluminum coils. Increased Fe content will reduce the cubic structure content; uneven distribution of Fe will lead to coarse grains, uneven corrosion, and deterioration of electrical properties of aluminum coils. Compared with its content, the presence and distribution of Fe have a greater impact on the performance of coated aluminum coils. The solubility of Fe in Al is extremely small. At different temperatures, Fe is soluble in Al and can also be segregated or precipitated in the form of particles such as FeAl₃ and FeAl6.

 

When more Fe is solid dissolved in the AI ​​matrix, it will hinder the migration of large-angle grain boundaries during the annealing process, inhibit the formation and growth of the cubic structure, and increase the recrystallization temperature, leading to the formation of the R texture, making the cubic texture structure content is reduced. When Fe precipitates in the form of FeAl₂ and FeAl6 compounds, it will deteriorate the performance of the corroded aluminum coil.

 

It can be seen that no matter what state Fe exists in high-purity aluminum, it is not conducive to the formation and growth of cubic structures during the annealing process of aluminum coils and the corrosion of aluminum coils. Therefore, manufacturing companies strictly control the Fe content during the production process of coated aluminum coils.

 

chemical composition table of coated-aluminium-coil

 

(2)The influence of Si.

The main source of Si impurities in high-purity aluminum is contamination from refractory materials. Si impurities are more difficult to control than Fe impurities. Excessive Si content will affect the growth of cubic texture, prone to over-dissolution, and will also cause coarse grains during aluminum recrystallization. Compared with Fe, Si has a greater solubility in Al and mainly exists in the form of solid solution. Its solid solution precipitation ability is weaker than that of Fe, and its adverse impact on the formation process of cubic texture is far less significant than that of Fe.

 

Si and Fe can influence each other's existence state when they coexist in high-purity aluminum. After adding Si to high-purity aluminum, the bulk diffusion rate of Fe increases, which can change the supersaturated solid solution state of Fe and the dispersion state of FeAl3, which is conducive to the formation and growth of cubic structures. The influence of Si on the performance of aluminum coils is also related to the content ratio of Si and Fe.

When the Fe content is low and the Si and Fe contents are relatively large, the electrostatic capacitance of the aluminum coil increases. When the Fe content is within (10~20)x10-6, the Si and Fe content ratio has a more significant impact on the electrostatic capacity of the aluminum coil. When the Fe content exceeds 30x10-6, it has no obvious effect on the electrostatic capacitance.

When the Si content is too high, the AI-Fe-Si ternary compound formed by excess Si has a higher potential than AI, which is not conducive to the dissolution of the Al matrix during corrosion formation. When the Si content exceeds 500x10-6, the formation time of the aluminum coil will be prolonged, and its continued increase will reduce the specific capacitance of the aluminum coil. Therefore, the Si content in coated aluminum coils is generally required to be controlled below 30x10-6.

 

aluminium-coils-alloy

 

(3) Influence of Cu.

Research has found that if the Cu content is too low, aluminum coils have poor corrosion resistance, and if the Cu content is too high, it will easily cause excessive corrosion. When the Cu content in high-purity aluminum increases, the electrostatic capacitance of the aluminum coil can be increased. When the Cu content reaches (27~30)x10-6, the increase in Cu content will reduce the specific capacitance of the aluminum coil. Umezawa Atsushi et al. studied the evolution of recrystallization texture in high-purity aluminum and found that when the Cu content in high-purity aluminum coils is 50x10-6, the cubic texture content in the recrystallization texture after annealing is Cu-free. twice the time, and no {123}<634>R texture was found. Lower Cu content and higher grain growth temperature are conducive to increasing the cubic texture content of high-purity aluminum coils. A certain amount of Cu can increase the porosity during the corrosion formation process of aluminum coils and increase the specific capacitance of aluminum coils. Therefore, domestic and foreign manufacturers generally add a certain amount of Cu to high-purity aluminum to increase the specific capacitance of aluminum coils. When the Cu content in high-purity aluminum coils is high, micro-batteries are easily formed in the working electrolyte of the coated aluminum coils, which will destroy the oxide film of the dielectric and worsen the performance of the capacitor. Therefore, the Cu content in high-purity aluminum coils should generally be controlled below 60x10-6.

 

Color-coating-aluminum-coil-process

 

(4) The influence of other trace elements.

Other main trace elements in aluminum coils include Mg, Be, Pb, Sn, Ni, Ti, etc. These solid solution trace elements are easy to segregate near the dislocations of aluminum, which will affect the crystallization of the aluminum coil in the subsequent rolling and annealing processes. It has an important impact on the formation of lattice, grain size, cubic texture formation, leakage current and corrosion process, which ultimately affects the performance of the capacitor, so its content must be strictly controlled.

 

Too much Mg will reduce the nucleation rate and nucleation speed of aluminum, which is not conducive to the formation and development of cubic texture. These trace elements will not always exist in the form of monomers in aluminum coils. As conditions change, they will form different types of compounds with other trace elements and AI to form solid solutions or precipitate. By studying the presence of trace elements in different forms of aluminum coils, their content in the aluminum coils can be effectively controlled. The presence of Mg will cause the lateral development of the corrosion tunnel of the aluminum coil, and can promote the peeling off of the corrosion tissue on the surface of the aluminum coil, which is not conducive to the improvement of its specific capacitance. At the same time, adding an appropriate amount of rare earth and Be can reduce the hindering effect of Fe on the formation of cubic texture in high-purity aluminum coils, promote the formation and growth of cubic texture, thereby increasing the cubic texture content.

 

At present, the better methods to control the content of trace elements are: adding trace amounts of rare earth (Y) to high-purity aluminum can change the relative strength of the deformed texture components in the aluminum coil; adding less Be can increase the cubic texture of the finished foil. structural strength. The solubility of rare earths and Be in Al is extremely small, and they can form a series of compounds with trace impurities such as Fe. After precipitation, the matrix can be purified, the concentration of Fe in the matrix is reduced, and the adverse effects of impurities on the cubic texture of the aluminum coil are eliminated. As the rare earth content increases, the orientation density of brass increases, the S texture component decreases, and the cubic texture content in the finished annealed foil decreases accordingly. When the rare earth content is 0.003%, the standard electrode potential of Pb2+ is significantly higher than AI+3. Adding Pb to high-purity aluminum coils can effectively increase the number of grains and corrosion pits, which is beneficial to corrosion on the surface of the aluminum coil, thus increasing the effective surface area of the aluminum coil. As the Pb content increases, the cubic texture content in the finished aluminum coil gradually decreases. When the Pb content reaches 0.3x10-6, the high-purity aluminum coil can obtain the maximum specific capacitance. Trace amounts of Pb in the aluminum coil will be concentrated on the surface of the aluminum coil, causing corrosion pores on the surface, thereby increasing the specific capacitance, and will not affect the strong cubic texture of the aluminum coil. Therefore, adding trace amounts of Pb can improve the performance of conventional lead-free aluminum coils. important technical means. However, Pb is a carcinogen. Mao Weimin and others studied using Sn to replace Pb and achieved good results.

 

When the Sn content in high-purity aluminum coils is below 20x10-6, the cubic texture content in the annealed aluminum coils can reach more than 95%, while when the Sn content exceeds 20x10-6, the cubic texture content in the aluminum coils will be reduced. . The effect of Sn content on the specific capacitance of aluminum coils is similar to that of Pb, so it can replace Pb to reduce environmental pollution.

In the production process of coated aluminum coils, not only the content of individual trace elements is limited, but also the total amount of other trace elements is required to be strictly controlled. In order to avoid adverse effects on the overall performance of coated aluminum coils, the content of other trace elements in coated aluminum coils should generally be controlled within 10x10-6.

 

coating-aluminium-coil